Difference between revisions of "Resists at QNF"
Jump to navigation
Jump to search
m (→Miscellaneous) |
|||
Line 66: | Line 66: | ||
! Name / Datasheet !! Tone !! Solvent Composition !! Use / Thickness !! Tool Compatibility !! Developer !! Remover | ! Name / Datasheet !! Tone !! Solvent Composition !! Use / Thickness !! Tool Compatibility !! Developer !! Remover | ||
|- | |- | ||
− | | [https://upenn.box.com/s/7ek7ccxq3c8xsp8jhe2lhdoi1e0keamt ZEP 520A] || + || Anisole || Thicker formulation || [https://wiki.nano.upenn.edu/wiki/index.php?title=Elionix_ELS-7500EX_E-Beam_Lithography_System EBL-01],[https://wiki.nano.upenn.edu/wiki/index.php?title=Elionix_ELS-7500EX_E-Beam_Lithography_System EBL-03], SPN-06 || Xylenes or Amyl acetate || NMP | + | | [https://upenn.box.com/s/7ek7ccxq3c8xsp8jhe2lhdoi1e0keamt ZEP 520A] || + || Anisole || Thicker formulation || [https://wiki.nano.upenn.edu/wiki/index.php?title=Elionix_ELS-7500EX_E-Beam_Lithography_System EBL-01], [https://wiki.nano.upenn.edu/wiki/index.php?title=Elionix_ELS-7500EX_E-Beam_Lithography_System EBL-03], SPN-06 || Xylenes or Amyl acetate || NMP |
|- | |- | ||
− | | [https://upenn.box.com/s/7ek7ccxq3c8xsp8jhe2lhdoi1e0keamt ZEP 520A-7] || + || Anisole || Thinner formulation || [https://wiki.nano.upenn.edu/wiki/index.php?title=Elionix_ELS-7500EX_E-Beam_Lithography_System EBL-01],[https://wiki.nano.upenn.edu/wiki/index.php?title=Elionix_ELS-7500EX_E-Beam_Lithography_System EBL-03], SPN-06 || Xylenes or Amyl acetate || NMP | + | | [https://upenn.box.com/s/7ek7ccxq3c8xsp8jhe2lhdoi1e0keamt ZEP 520A-7] || + || Anisole || Thinner formulation || [https://wiki.nano.upenn.edu/wiki/index.php?title=Elionix_ELS-7500EX_E-Beam_Lithography_System EBL-01], [https://wiki.nano.upenn.edu/wiki/index.php?title=Elionix_ELS-7500EX_E-Beam_Lithography_System EBL-03], SPN-06 || Xylenes or Amyl acetate || NMP |
|- | |- | ||
− | | [https://upenn.box.com/s/bv53alommdr2en6s6byrlm4psxdjohzp H-SiQ 6%] || - || MIBK || HSQ Equivalent || [https://wiki.nano.upenn.edu/wiki/index.php?title=Elionix_ELS-7500EX_E-Beam_Lithography_System EBL-01],[https://wiki.nano.upenn.edu/wiki/index.php?title=Elionix_ELS-7500EX_E-Beam_Lithography_System EBL-03], SPN-06 || TMAH || | + | | [https://upenn.box.com/s/bv53alommdr2en6s6byrlm4psxdjohzp H-SiQ 6%] || - || MIBK || HSQ Equivalent || [https://wiki.nano.upenn.edu/wiki/index.php?title=Elionix_ELS-7500EX_E-Beam_Lithography_System EBL-01], [https://wiki.nano.upenn.edu/wiki/index.php?title=Elionix_ELS-7500EX_E-Beam_Lithography_System EBL-03], SPN-06 || TMAH || |
|} | |} | ||
Revision as of 15:42, 24 May 2024
The QNF provides a variety of standard resists to meet demands for most applications. Some specialty resists are also sold through the QNF Stockroom. A summary of stocked resists along with some processing information can be found in the table below. Click on the resist name to access the datasheet. Other similar options that may be available in QNF are also listed.
QNF Supplied Standard Photoresists
Name / Datasheet | Tone | Solvent Composition | Use / Thickness | Tool Compatibility | Developer | Remover | Alternative Resists |
---|---|---|---|---|---|---|---|
S1805 | + | PGMEA | General | MA-01, LW-01, SPN-01, SPN-03 |
TMAH | NMP | KL5305 |
S1813 | + | PGMEA | General, 1um-1.3um | MA-01, LW-01, SPN-01, SPN-03, RC-01 |
TMAH | NMP | KL5315 |
S1818 | + | PGMEA | General | MA-01, LW-01, SPN-01, SPN-03 |
TMAH | NMP | |
SPR 220-3 | + | Ethyl lactate, anisole, n-amyl acetate | Etch, 2um-5um | MA-01, SPN-01, SPN-03 |
TMAH | NMP | KPRO-3, KL6003, AZ3330F |
SPR 220-4.5 | + | Ethyl lactate, anisole, n-amyl acetate | Etch | MA-01, SPN-01, SPN-03 |
TMAH | NMP | KPRO-3, KL6003, AZ3330F |
SPR 220-7 | + | Ethyl lactate, anisole, n-amyl acetate | Etch, 6um-12um | MA-01, SPN-01, SPN-03 |
TMAH | NMP | AZ 12XT, AZ P4620 |
AZ 3330F | + | PGMEA | General, Metal RIE, Plating | MA-01, SPN-01, SPN-03 |
TMAH or AZ400K 1:4 | SPR 220-3, SPR 220-4.5, K-PRO 3, KL6003 | |
NR7-3000P | - | Cyclohexanone | Etch, General | MA-01, SPN-01, SPN-03, SPN-04 |
TMAH | ||
APOL-LO 3202 | - | PGMEA | Liftoff | MA-01, SPN-01, SPN-03, SPN-04, RC-01 |
TMAH | NMP | |
IP-Dip | - | Ethoxylated acrylates | Nanoscribe, Epoxy | LW-02 | PGMEA (SU-8 or HARE SQ Developer), IPA | N/A | |
HARE SQ 2 | - | Cyclopentanone, gamma butyro lactone | Epoxy, 2um-5um | MA-01, MA-03, SPN-04, SPN-08 |
PGMEA (SU-8 or HARE SQ Developer), IPA | N/A | SU-8 2005 |
HARE SQ 50 | - | Cyclopentanone, gamma butyro lactone | Epoxy, 25um-100um | MA-01, MA-03, SPN-04, SPN-08 |
PGMEA (SU-8 or HARE SQ Developer), IPA | N/A | SU-8 2050 |
Stockroom Photoresists
Name / Datasheet | Tone | Solvent Composition | Use / Thickness | Tool Compatibility | Developer | Remover | Alternative Resists |
---|---|---|---|---|---|---|---|
SU-8 2005 | - | Cyclopentanone | Epoxy, 4um-7um | MA-01, MA-03, SPN-04, SPN-08 | PGMEA (SU-8 or SQ Developer) | N/A | HARE SQ 2 |
SU-8 2050 | - | Cyclopentanone | Epoxy, 40um-170um | MA-01, MA-03, SPN-04, SPN-08 | PGMEA (SU-8 or SQ Developer) | N/A | HARE SQ 50 |
SU-8 2100 | - | Cyclopentanone | Epoxy, 100um-270um | MA-01, MA-03, SPN-04, SPN-08 | PGMEA (SU-8 or SQ Developer) | N/A | HARE SQ 50 |
SU-8 3050 | - | Cyclopentanone | Epoxy, 40um-100um | MA-01, MA-03, SPN-04, SPN-08 | PGMEA (SU-8 or SQ Developer) | N/A | HARE SQ 50 |
Standard e-beam Resists
Name / Datasheet | Tone | Solvent Composition | Use / Thickness | Tool Compatibility | Developer | Remover | Alternative Resists |
---|---|---|---|---|---|---|---|
495 PMMA A8 | + | Anisole | Lower Resolution | EBL-01, EBL-03, SPN-06 | 3:1 IPA/H2O | NMP | |
495 PMMA A4 | + | Anisole | Lower Resolution, 180nm-300nm | EBL-01, EBL-03, SPN-06 | 3:1 IPA/H2O | NMP | |
495 PMMA A2 | + | Anisole | Lower Resolution, 50nm-100nm | EBL-01,EBL-03, SPN-06 | 3:1 IPA/H2O | NMP | |
950 PMMA A4 | + | Anisole | High Resolution, 200nm-400nm | EBL-01,EBL-03, SPN-06 | 3:1 IPA/H2O | NMP | |
950 PMMA A2 | + | Anisole | High Resolution, 50nm-100nm | EBL-01,EBL-03, SPN-06 | 3:1 IPA/H2O | NMP | 1000 HARP 0.1 |
1000 HARP 1.3 | + | Anisole | High Resolution | EBL-01,EBL-03, SPN-06 | 3:1 IPA/H2O | NMP | |
1000 HARP 0.1 | + | Anisole | High Resolution | EBL-01,EBL-03, SPN-06 | 3:1 IPA/H2O | NMP | 950 PMMA A2 |
Stockroom e-beam Resists
Name / Datasheet | Tone | Solvent Composition | Use / Thickness | Tool Compatibility | Developer | Remover |
---|---|---|---|---|---|---|
ZEP 520A | + | Anisole | Thicker formulation | EBL-01, EBL-03, SPN-06 | Xylenes or Amyl acetate | NMP |
ZEP 520A-7 | + | Anisole | Thinner formulation | EBL-01, EBL-03, SPN-06 | Xylenes or Amyl acetate | NMP |
H-SiQ 6% | - | MIBK | HSQ Equivalent | EBL-01, EBL-03, SPN-06 | TMAH |
Other Resists
Name / Datasheet | Tone | Solvent Composition | Use / Thickness | Tool Compatibility | Developer | Remover |
---|---|---|---|---|---|---|
LOR 3A | N/A | Cyclopentanone, PGME | Liftoff, Non-imaging | SPN-03, SPN-04 only! Precipitates in acetone, PGMEA |
TMAH | NMP |
PMGI SF 5S | N/A | Cyclopentanone, PGME | Liftoff, Non-imaging | SPN-03, SPN-04 only! Precipitates in acetone, PGMEA |
TMAH | NMP |
PMGI SF 2S | N/A | Cyclopentanone, PGME | Liftoff, Non-imaging | SPN-03, SPN-04 only! Precipitates in acetone, PGMEA |
TMAH | NMP |
NXR-1025 | N/A | Proprietary | Stockroom, Nanoimprint | MA-02 |
Miscellaneous
These may be available but are not guaranteed to be stocked
Name / Datasheet | Tone | Solvent Composition | Use / Thickness | Tool Compatibility | Developer | Remover | Alternative Resists |
---|---|---|---|---|---|---|---|
KL5305 | + | PGMEA | General | MA-01, SPN-01, SPN-03 | TMAH | NMP | S1805 |
KL5315 | + | PGMEA | General | MA-01, SPN-01, SPN-03 | TMAH | NMP | S1813 |
KL6003 | + | PGMEA | MA-01, SPN-01, SPN-03 | TMAH | NMP | SPR 220-3, SPR 220-4.5 | |
K-PRO 3 | + | PGMEA | Plating, Etching | MA-01, SPN-01, SPN-03 | TMAH or AZ400K 1:4 | NMP | SPR 220-3, SPR 220-4.5 |
AZ 12XT-20PL-15 | + | PGMEA | CAR (i-line), Plating, Packaging, Deep Etch, 10um-25um | MA-01, SPN-01, SPN-03 | TMAH | SPR 220-7, AZ P4620 | |
AZ P4620 | + | PGMEA | Thick Resist, Plating, Packaging | MA-01, SPN-01, SPN-03 | TMAH or AZ400K 1:4 | SPR 220-7, AZ 12XT-20PL-15 | |
ma-N 2403 | - | NMP, Butyl acetate, Cyclohexanone | e-beam/DUV Mix and Match | EBL-01, EBL-03, SPN-06 |