W master recipe
Jump to navigation
Jump to search
> Click here to return to PVD-05 <
Step T010 is the deposition step.
Step Number | T000 | T001 | T002 | T003 | T004 | T005 | T006 | T007 | T008 | T009 | T010 | T011 | T012 |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Step Time (sec) | 5 | 60 | 60 | 60 | 60 | 60 | 60 | 60 | 60 | 60 | [dep] | 200 | 5 |
Min Vacuum Setpoint (Torr) | |||||||||||||
Gas - (PID or Fixed) | PID | PID | PID | PID | PID | PID | PID | PID | PID | PID | |||
Gas - PID Master Gas Select | 1 | 1 | 1 | 1 | 1 | 1 | 1 | 1 | 1 | 1 | |||
Gas1 - Setpoint (sccm) | 30 | 30 | 30 | 30 | 30 | 30 | 30 | 30 | 30 | 30 | |||
Gas2 - Setpoint (sccm) | |||||||||||||
Gas PID Pressure (mTorr) | 30 | 25 | 20 | 15 | 12 | 10 | 8 | 6 | 4 | 3 | |||
RF Source - Sputter (Watts) | |||||||||||||
RF Source - Cathode Select | |||||||||||||
RF Source - Shutter | |||||||||||||
DC 1 Source - Sputter (Watts) | 100 | 100 | 100 | 150 | 200 | 250 | 300 | 350 | 400 | 450 | |||
DC 1 Source - Cathode Select | 1 | 1 | 1 | 1 | 1 | 1 | 1 | 1 | 1 | 1 | |||
DC 1 Source - Shutter | Open | ||||||||||||
DC 2 Source - Sputter (Watts) | |||||||||||||
DC 2 Source - Shutter | |||||||||||||
Pressure Control (Throttle) | Yes | Yes | Yes | Yes | Yes | Yes | Yes | Yes | Yes | Yes | Yes | ||
Ignition Pressure (mTorr) | |||||||||||||
Rotation Speed (0-100%) | 50 | 50 | 50 | 50 | 50 | 50 | 50 | 50 | 50 | 50 | 50 | 50 | |
End Process (Yes) | Yes |