Difference between revisions of "Ag master recipe"

From Quattrone Nanofabrication Facility
Jump to navigation Jump to search
 
(7 intermediate revisions by the same user not shown)
Line 1: Line 1:
===== Silver (Ag) =====
+
> [[Denton_Explorer14_Magnetron_Sputterer#Process_data_&_master_recipes | Click here to return to PVD-05]]  <
  
Note the extra long cool-down time. Reducing this time can affect the target.
+
Step T006 is the deposition step. Note the extra long cool-down time in step T012. Reducing the cool-down time will result in significant surface oxidation. Please do not alter this time.
  
 
{| class="wikitable"
 
{| class="wikitable"
! Step Number || T000 || T001 || T002 || T003 || T004 || T005 || T006
+
! Step Number || T000 || T001 || T002 || T003 || T004 || T005 || T006 || T007 || T008 || T009 || T010 || T011 || T012 || T013
 
|-
 
|-
 
|-
 
|-
| Step Time (sec) || - || || - || - || - || - || -
+
| Step Time (sec) || 5 || 30 || 30 || 30 || 30 || 30 || [dep] || 30 || 30 || 30 || 30 || 30 || 900 || 5
 
|-style="background-color:#FFFFFF"  
 
|-style="background-color:#FFFFFF"  
| Min Vacuum Setpoint (Torr) || - || - || - || - || - || - || -
+
| Min Vacuum Setpoint (Torr) || ||  || ||  || || ||  ||  ||  ||  ||  ||  ||  ||  
 
|-
 
|-
|  ||  ||   ||  ||  ||  ||  ||  
+
|  ||  || ||  ||  ||  ||  ||  ||  ||  || ||  ||  ||  || 
 
|-style="background-color:#DBFEFF"  
 
|-style="background-color:#DBFEFF"  
| Gas - (PID or Fixed) || - || - || - || - || - || - || -
+
| Gas - (PID or Fixed) || || PID || PID || PID || PID || PID || PID || PID || PID || PID || PID || PID || ||  
 
|-style="background-color:#FFFFFF"
 
|-style="background-color:#FFFFFF"
| Gas - PID Master Gas Select || - || - || - || - || - || - || -
+
| Gas - PID Master Gas Select || || 1 || 1 || 1 || 1 || 1 || 1 || 1 || 1 || 1 || 1 || 1 ||  ||  
 
|-  
 
|-  
| Gas1 - Setpoint (sccm) || - || - || - || - || - || - || -
+
| Gas1 - Setpoint (sccm) || || 10 || 10 || 10 || 10 || 10 || 10 || 10 || 10 || 10 || 10 || 10 || ||
 
|-style="background-color:#FFFFFF"
 
|-style="background-color:#FFFFFF"
| Gas2 - Setpoint (sccm) || - ||  - || - || - || - || - || -
+
| Gas2 - Setpoint (sccm) ||  ||  || ||  || || || || ||  ||  ||  ||  ||  ||  
 
|-
 
|-
|  ||  ||   ||  ||  ||  ||  ||  
+
|  ||  || ||  ||  ||  ||  ||  ||  ||  ||  ||  ||  ||  ||  
 
|-style="background-color:#DEB4DC"  
 
|-style="background-color:#DEB4DC"  
|Gas PID Pressure (mTorr) || - || - || - || - || - || - || -
+
|Gas PID Pressure (mTorr) || || 3 || 3 || 3 || 3 || 3 || 3 || 3 || 3 || 3 || 3 || 3 || ||
 
|-style="background-color:#DCF5E9"  
 
|-style="background-color:#DCF5E9"  
| RF Source - Sputter (Watts) || - || - || - || - || - || - || -
+
| RF Source - Sputter (Watts) || || || || || || ||  ||  ||  ||  ||  ||  ||  ||  
 
|-style="background-color:#DCF5E9"  
 
|-style="background-color:#DCF5E9"  
| RF Source - Cathode Select || - ||  - || - || - || - || - || -
+
| RF Source - Cathode Select ||  ||  || ||  || || || || ||  ||  ||  ||  ||  ||  
 
|-style="background-color:#DCF5E9"  
 
|-style="background-color:#DCF5E9"  
| RF Source - Shutter || - ||  - || - || - || - || - || -
+
| RF Source - Shutter ||  ||  || ||  || || || || ||  ||  ||  ||  ||  ||  
 
|-style="background-color:#ECFA6F"  
 
|-style="background-color:#ECFA6F"  
| DC 1 Source - Sputter (Watts) || - || - || - || - || - || - || -
+
| DC 1 Source - Sputter (Watts) || || 25 || 50 || 75 || 100 || 125 || 140 || 120 || 100 || 80 || 60 || 25 ||  ||
 
|-style="background-color:#ECFA6F"  
 
|-style="background-color:#ECFA6F"  
| DC 1 Source - Cathode Select || - || - || - || - || - || - || -
+
| DC 1 Source - Cathode Select || || 1 || 1 || 1 || 1 || 1 || 1 || 1 || 1 || 1 || 1 || 1 ||  ||
 
|-style="background-color:#ECFA6F"  
 
|-style="background-color:#ECFA6F"  
| DC 1 Source - Shutter || - || - || - || - || - || - || -
+
| DC 1 Source - Shutter || || || || || || || Open ||  ||  ||  ||  ||  ||  ||
 
|-style="background-color:#FAD86F"  
 
|-style="background-color:#FAD86F"  
| DC 2 Source - Sputter (Watts) || - ||  - || - || - || - || - || -
+
| DC 2 Source - Sputter (Watts) || ||  ||  ||  ||  ||  || || || || ||  ||  ||  ||  
 
|-style="background-color:#FAD86F"
 
|-style="background-color:#FAD86F"
|  ||  ||  ||  ||  ||  ||  ||  
+
|  ||  ||  ||  ||  ||  ||  || ||  ||  ||  ||  ||  ||  || 
 
|-style="background-color:#FAD86F"
 
|-style="background-color:#FAD86F"
| DC 2 Source - Shutter || - || - || - || - || - || - || -
+
| DC 2 Source - Shutter || || || || || || ||  ||  ||  ||  ||  ||  ||  ||  
 
|-style="background-color:#6FD2FA"  
 
|-style="background-color:#6FD2FA"  
| Pressure Control (Throttle) || - || - || - || - || - || - || -
+
| Pressure Control (Throttle) || Yes || Yes || Yes || Yes || Yes || Yes || Yes || Yes || Yes || Yes || Yes || Yes || ||  
 
|-style="background-color:#FFFFFF"
 
|-style="background-color:#FFFFFF"
| Ignition Pressure (mTorr) || - ||  - || - || - || - || - || -
+
| Ignition Pressure (mTorr) || ||  ||  ||  ||  ||  || || || || ||  ||  ||  ||  
 
|-
 
|-
|  ||  ||   ||  ||  ||  ||  ||  
+
|  ||  || ||  ||  ||  ||  ||  ||  ||  ||  ||  ||  ||  ||  
 
|-style="background-color:#E8F213"  
 
|-style="background-color:#E8F213"  
| Rotation Speed (0-100%) || - || - || - || - || - || - || -
+
| Rotation Speed (0-100%) || 50 || 50 || 50 || 50 || 50 || 50 || 50 || 50 || 50 || 50 || 50 || 50 || 50 ||  
 
|-
 
|-
| End Process (Yes) || - ||  - || - || - || - || - || -
+
| End Process (Yes) || ||  ||  ||  ||  ||  || || || || ||  ||  ||  || Yes
 
|}
 
|}

Latest revision as of 11:27, 31 January 2023

> Click here to return to PVD-05 <

Step T006 is the deposition step. Note the extra long cool-down time in step T012. Reducing the cool-down time will result in significant surface oxidation. Please do not alter this time.

Step Number T000 T001 T002 T003 T004 T005 T006 T007 T008 T009 T010 T011 T012 T013
Step Time (sec) 5 30 30 30 30 30 [dep] 30 30 30 30 30 900 5
Min Vacuum Setpoint (Torr)
Gas - (PID or Fixed) PID PID PID PID PID PID PID PID PID PID PID
Gas - PID Master Gas Select 1 1 1 1 1 1 1 1 1 1 1
Gas1 - Setpoint (sccm) 10 10 10 10 10 10 10 10 10 10 10
Gas2 - Setpoint (sccm)
Gas PID Pressure (mTorr) 3 3 3 3 3 3 3 3 3 3 3
RF Source - Sputter (Watts)
RF Source - Cathode Select
RF Source - Shutter
DC 1 Source - Sputter (Watts) 25 50 75 100 125 140 120 100 80 60 25
DC 1 Source - Cathode Select 1 1 1 1 1 1 1 1 1 1 1
DC 1 Source - Shutter Open
DC 2 Source - Sputter (Watts)
DC 2 Source - Shutter
Pressure Control (Throttle) Yes Yes Yes Yes Yes Yes Yes Yes Yes Yes Yes Yes
Ignition Pressure (mTorr)
Rotation Speed (0-100%) 50 50 50 50 50 50 50 50 50 50 50 50 50
End Process (Yes) Yes