! Name || Pulse time [s] || Wait time [s] || Name || Pulse time [s] || Wait time [s]  
 
! Name || Pulse time [s] || Wait time [s] || Name || Pulse time [s] || Wait time [s]  
 
|-  
 
|-  
| Al<sub>2</sub>O<sub>3</sub> || TMA || 0.015 || 5 || O<sub>3</sub> || 0.05 || 5 || 200 || 20 || 1 || 09/24/22
+
| Al<sub>2</sub>O<sub>3</sub> || TMA || 0.015 || 5 || O<sub>3</sub> || 0.05 || 5 || 200 || 20 || 1.1 || 10/17/22
 
|-
 
|-
| HfO<sub>2</sub> || TDMAHf || 0.15 || 8 || H<sub>2</sub>O || 0.015 || 5 || 200 || 20 || 1.3 || 09/24/22
+
| Pt || Pt precursor || 0.6 || 5 || O<sub>3</sub> || 0.05 || 5 || 200 || 20 || 0.7 || 10/18/22
 
|-
 
|-
 
|}
 
|}
 +
 +
Note that Pt deposition saturates at ~ 10 nm and the deposition rate only applies to thicknesses of ~ 5 - 10nm.

Revision as of 14:10, 18 October 2022


Creating Veeco Savannah 200
ALD-03.jpeg
Tool Name Creating Veeco Savannah 200
Instrument Type Deposition
Staff Manager Sam Azadi
Lab Location Bay 2
Tool Manufacturer Veeco
Tool Model Savannah 200
NEMO Designation {{{NEMO_Designation}}}
Nearest Phone 215-898-9736
SOP Link SOP

Description

Savannah is equipped with high-speed pneumatic pulse valves to enable our unique Exposure Mode for thin film deposition on Ultra High Aspect Ratio substrates. This proven precision thin film coating methodology can be used to deposit conformal, uniform films on substrates with aspect ratios of greater than > 2000:1. Savannah is capable of holding substrates of different sizes up to 200mm. The Savannah thin film deposition systems are equipped with Pd, Pt precursors, TMA, HfCl4, formalin and Ozone.

Films
  • Pt
  • Aluminum oxide
  • Pd
  • Under development: Hafnia (using HfCl4 and O3)

Resources

SOPs & Troubleshooting
Most Recent Deposition Rates
Material Name Precursor 1 Precursor 2 Dep. temperature [C] Carrier flow [sccm] Dep. rate [A/cyc] Date [MM/DD/YY]
Name Pulse time [s] Wait time [s] Name Pulse time [s] Wait time [s]
Al2O3 TMA 0.015 5 O3 0.05 5 200 20 1.1 10/17/22
Pt Pt precursor 0.6 5 O3 0.05 5 200 20 0.7 10/18/22

Note that Pt deposition saturates at ~ 10 nm and the deposition rate only applies to thicknesses of ~ 5 - 10nm.