Difference between revisions of "SUSS MicroTec MA6 Gen3 Mask Aligner"
m (Changed protection level for "SUSS MicroTec MA6 Gen3 Mask Aligner" ([Edit=Allow only autoconfirmed users] (indefinite) [Move=Allow only autoconfirmed users] (indefinite))) |
(Including suggested exposure parameters based on datasheets, including description of wavelength selection.) |
||
Line 22: | Line 22: | ||
* Photomask exposure of resist-coated samples | * Photomask exposure of resist-coated samples | ||
+ | |||
+ | == Processes == | ||
+ | The following may be used as guidelines to determine exposure parameters based on resist type and thickness. Information based on the following resist datasheets -- | ||
+ | [https://amolf.nl/wp-content/uploads/2016/09/datasheets_S1800.pdf S1800 Series], | ||
+ | [https://kayakuam.com/wp-content/uploads/2019/09/SPR-220-DATA-SHEET-RH.pdf SPR 220 Series], | ||
+ | [https://kayakuam.com/wp-content/uploads/2019/09/SU-82000DataSheet2000_5thru2015Ver4-2.pdf SU-8 2000-2015], | ||
+ | [https://kayakuam.com/wp-content/uploads/2019/09/SU-82000DataSheet2025thru2075Ver4-1.pdf SU-8 2025-2075], | ||
+ | [https://kayakuam.com/wp-content/uploads/2019/09/SU-82000DataSheet2100and2150Ver5.pdf SU-8 2100], | ||
+ | [https://kayakuam.com/wp-content/uploads/2020/07/KAM-SU-8-3000-Datasheet-7.10-final.pdf SU-8 3000]. | ||
+ | |||
+ | |||
+ | {| class="wikitable" style="vertical-align:bottom;" | ||
+ | |- | ||
+ | ! Resist | ||
+ | ! Thickness (um) | ||
+ | ! Dose (mJ/cm2) | ||
+ | ! Channel | ||
+ | |- | ||
+ | | S1813 | ||
+ | | 1.2 | ||
+ | | 150 | ||
+ | | #2 | ||
+ | |- | ||
+ | | SPR220 - 3.0 | ||
+ | | 3.0 | ||
+ | | 310 | ||
+ | | #1 | ||
+ | |- | ||
+ | | SPR220 - 4.5 | ||
+ | | 5.0 | ||
+ | | 380 | ||
+ | | #1 | ||
+ | |- | ||
+ | | SU-8 2005 | ||
+ | | 5.0 - 6.0 | ||
+ | | 105 - 110 | ||
+ | | #1 | ||
+ | |- | ||
+ | | SU-8 2050 | ||
+ | | 40 - 80 | ||
+ | | 150 - 215 | ||
+ | | #1 | ||
+ | |- | ||
+ | | SU-8 2050 | ||
+ | | 80 - 110 | ||
+ | | 215 - 240 | ||
+ | | #1 | ||
+ | |- | ||
+ | | SU-8 2050 | ||
+ | | 115 - 160 | ||
+ | | 240 - 260 | ||
+ | | #1 | ||
+ | |- | ||
+ | | SU-8 2100 | ||
+ | | 100 - 150 | ||
+ | | 240 - 260 | ||
+ | | #1 | ||
+ | |- | ||
+ | | SU-8 2100 | ||
+ | | 150 - 225 | ||
+ | | 260 - 350 | ||
+ | | #1 | ||
+ | |- | ||
+ | | SU-8 2100 | ||
+ | | 225 - 270 | ||
+ | | 350 - 370 | ||
+ | | #1 | ||
+ | |- | ||
+ | | SU-8 3050 | ||
+ | | 40 - 100 | ||
+ | | 150 - 250 | ||
+ | | #1 | ||
+ | |} | ||
+ | |||
+ | ===== Exposure Wavelengths ===== | ||
+ | |||
+ | The software adjusts the lamp intensity controller during exposure based on the channel selected in the recipe. | ||
+ | * Channel #1 = 365nm (i-line) | ||
+ | * Channel #2 = 405nm (h-line) | ||
+ | |||
+ | For some applications it can be beneficial to eliminate wavelengths below 365nm using a long pass filter. ''' ''Contact staff to be trained on setting this filter if you plan to use it.'' ''' Since higher energy wavelengths are removed, expect an increase in exposure time of approximately 40% to reach the optimum exposure dose. | ||
== Resources == | == Resources == |
Revision as of 16:20, 29 June 2023
![]() |
|
Tool Name | SUSS MicroTec MA6 Gen3 Mask Aligner |
---|---|
Instrument Type | Lithography |
Staff Manager | David Jones |
Lab Location | Bay 2 |
Tool Manufacturer | SUSS MicroTec |
Tool Model | MA6 Gen3 |
NEMO Designation | {{{NEMO_Designation}}} |
Lab Phone | XXXXX |
SOP Link | SOP |
Description
This system is a dual-use mask aligner and wafer-bond aligner. Mask alignment is used for contact and proximity exposure processes. Exposures can be performed with gaps programmable from 10 um to 300 um in 1 um increments. Automatic wedge error compensation (WEC) is used to ensure that the mask and wafer are parallel. The lamp is a 1000 W Hg-Arc lamp. Integrated light level sensing ensures proper exposure doses as the lamp degrades.
Applications
- Photomask exposure of resist-coated samples
Processes
The following may be used as guidelines to determine exposure parameters based on resist type and thickness. Information based on the following resist datasheets -- S1800 Series, SPR 220 Series, SU-8 2000-2015, SU-8 2025-2075, SU-8 2100, SU-8 3000.
Resist | Thickness (um) | Dose (mJ/cm2) | Channel |
---|---|---|---|
S1813 | 1.2 | 150 | #2 |
SPR220 - 3.0 | 3.0 | 310 | #1 |
SPR220 - 4.5 | 5.0 | 380 | #1 |
SU-8 2005 | 5.0 - 6.0 | 105 - 110 | #1 |
SU-8 2050 | 40 - 80 | 150 - 215 | #1 |
SU-8 2050 | 80 - 110 | 215 - 240 | #1 |
SU-8 2050 | 115 - 160 | 240 - 260 | #1 |
SU-8 2100 | 100 - 150 | 240 - 260 | #1 |
SU-8 2100 | 150 - 225 | 260 - 350 | #1 |
SU-8 2100 | 225 - 270 | 350 - 370 | #1 |
SU-8 3050 | 40 - 100 | 150 - 250 | #1 |
Exposure Wavelengths
The software adjusts the lamp intensity controller during exposure based on the channel selected in the recipe.
- Channel #1 = 365nm (i-line)
- Channel #2 = 405nm (h-line)
For some applications it can be beneficial to eliminate wavelengths below 365nm using a long pass filter. Contact staff to be trained on setting this filter if you plan to use it. Since higher energy wavelengths are removed, expect an increase in exposure time of approximately 40% to reach the optimum exposure dose.