− | ! rowspan=2 | | + | ! rowspan=2 | PVD Tool |
! colspan=3 | Cathode 2 (DC; high mag) | ! colspan=3 | Cathode 2 (DC; high mag) | ||
! rowspan=2 | Recorded | ! rowspan=2 | Recorded | ||
Line 30: | Line 30: | ||
! Pressure || Power || Rate || Pressure || Power || Rate || Pressure || Power || Rate | ! Pressure || Power || Rate || Pressure || Power || Rate || Pressure || Power || Rate | ||
|- | |- | ||
− | | | + | | PVD-03 || 6 mTorr || 300 W || 1.8 Å s<sup>-1</sup> || || 5 mTorr || 300 W || 0.98 Å s<sup>-1</sup> || 03/06/23 || 6 mTorr || 300 W || 0.8 Å s<sup>-1</sup> || |
+ | |- | ||
+ | |} | ||
+ | |||
+ | {| class="wikitable" | ||
+ | ! rowspan=2 | PVD Tool | ||
+ | ! colspan=3 | Cathode 2 (DC; high mag) | ||
+ | ! rowspan=2 | Recorded | ||
+ | |- | ||
+ | ! Pressure || Power || Rate || Pressure || Power || Rate || Pressure || Power || Rate | ||
+ | |- | ||
+ | | PVD-05 || 3 mTorr || 350 W || 2.0 Å s<sup>-1</sup> || | ||
|- | |- | ||
|} | |} |
Revision as of 13:42, 9 May 2024
Titanium is a transition metal with atomic number 22 and symbol Ti. Titanium has a low density, high strength and is resistant to corrosion by water. It has relatively poor electrical and thermal conduction compared to most metals.
Equipment
Deposition Equipment
- PVD-02: Lesker PVD75 E-Beam/Thermal Evaporator
- PVD-04: Lesker PVD75 E-beam Evaporator
- PVD-03: Lesker PVD75 DC/RF Sputterer
- PVD-05: Denton Explorer14 Magnetron Sputterer
Etching
Application
Processes
Sputter Deposition Rates
PVD Tool | Cathode 2 (DC; high mag) | Recorded | Cathode 3 (DC) | Recorded | Cathode 4 (DC; high mag) | Recorded | ||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|
Pressure | Power | Rate | Pressure | Power | Rate | Pressure | Power | Rate | ||||
PVD-03 | 6 mTorr | 300 W | 1.8 Å s-1 | 5 mTorr | 300 W | 0.98 Å s-1 | 03/06/23 | 6 mTorr | 300 W | 0.8 Å s-1 |
PVD Tool | Cathode 2 (DC; high mag) | Recorded | ||||||
---|---|---|---|---|---|---|---|---|
Pressure | Power | Rate | Pressure | Power | Rate | Pressure | Power | Rate |
PVD-05 | 3 mTorr | 350 W | 2.0 Å s-1 |