Description

The fully automated DWL 66+ laser writing system has both binary (2D) and grayscale (2.5D) exposure capability. The pattern is broken into vertical stripes of ~500px with preset overlap. To write each stripe, the tool modulates and deflects the laser beam based on the provided pattern data while the stage moves along Y. This process repeats along the X direction until the pattern is complete.

Schematic of pattern exposure with the DWL66+ Source -- TheLithographer.com, Surface Issue, May 2025

Lens & Resolution

  • 2 mm lens : 600 nm
  • 10 mm lens : 2 µm
  • 40 mm lens : 10 µm
Applications
Allowed Materials
  • Mask Plates -- available in the QNF Stockroom pre-coated with AZ1500 and IP3500
  • Resists -- must be compatible with h-line/ 405nm exposure (Laser exchanged in June 2023. Previous documentation may include 365nm capability.)

Processes

Writehead Selection

Pneumatic mode not recommended for dry etch and smaller features due to focus issues -- currently working with Heidelberg service to address.
Last confirmed July 2025.

Write Head Focus Mode Notes
10mm -100 Pneumatic active problem, see note above
10mm -70 Optical for >2um minimum
2mm -100 Pneumatic active problem, see note above
2mm +40 Optical for >600nm minimum
40mm -100 Pneumatic active problem, see note above

Photomask Exposure

500nm resist thickness on chrome-coated soda lime. Development in TMAH 0.26N for 60s.
Last confirmed July 2025.

Mask Write Head Filter(s) Laser Power Intensity Notes
AZ1500 10mm 50% 60 mW 90
IP3500 10mm NONE 120 mW 90 for <3um
AZ1500 2mm 12.5% + 25% 60 mW 80
IP3500 2mm 12.5% + 50% 60 mW 80 for <1um
AZ1500 40mm NONE 220 mW 60

Other direct write exposures

Resist on 4" silicon wafer, soft baked at 115C for 60s, development in TMAH 0.26N for 60s.
Due to the variability of resist thickness, substrate reflectivity, and the ideal profile for subsequent processes, a dose test is always recommended to confirm optimal parameters.

Resist Thickness/Spin Speed Write Head Filter(s) Laser Power Intensity
S1805 0.5um (3krpm) 10mm 50% 60 mW 70
S1818 2.2um (3krpm) 10mm NONE 130 mW 100


 LW-01 S1818Lines 25um Feb2024.png LW-01 S1818Lines 5um Feb2024.png
 S1818 at 3000rpm (2.2um thickness) with 10mm writehead [Feb 2024]
 65mW, NO Filter, 70% intensity, + 20 focus
 5um, 10um, 25um, and 50um line widths after 60s TMAH 0.26N development