Difference between revisions of "Cambridge Nanotech S200 ALD"
Jump to navigation
Jump to search
Line 44: | Line 44: | ||
===== Most Recent Deposition Rate ===== | ===== Most Recent Deposition Rate ===== | ||
− | {| class="wikitable | + | {| class="wikitable" |
− | ! Material Name ! | + | ! rowspan=2 |Material Name |
− | + | ! colspan=3 |Precursor 1 | |
+ | ! colspan =3 |Precursor 2 | ||
+ | ! rowspan=2 |Dep. temperature [C] | ||
+ | !rowspan=2 | Carrier flow [sccm] | ||
+ | !rowspan=2 | Dep. rate [A/cyc] | ||
+ | !rowspan=2 |Date [MM/DD/YY] | ||
|- | |- | ||
− | | Al<sub>2</sub>O<sub>3</sub> || TMA || H<sub>2</sub>O | + | ! Name || Pulse time [s] || Wait time [s] || Name || Pulse time [s] || Wait time [s] |
+ | |- | ||
+ | | Al<sub>2</sub>O<sub>3</sub> || TMA || 0.015 || 5 || H<sub>2</sub>O || 0.015 || 5 || 200 || 20 || 1 || 09/24/22 | ||
+ | |- | ||
+ | | HfO<sub>2</sub> || TDMAHf || 0.15 || 8 || H<sub>2</sub>O || 0.015 || 5 || 200 || 20 || 1.3 || 09/24/22 | ||
+ | |- | ||
+ | | TiO<sub>2</sub> || TDMATi || 0.4 || 10 || H<sub>2</sub>O || 0.015 || 5 || 250 || 20 || 0.4 || 05/02/22 | ||
|- | |- | ||
− | |||
|} | |} |
Revision as of 11:18, 27 September 2022
![]() |
|
Tool Name | Cambridge Nanotech S200 ALD |
---|---|
Instrument Type | Deposition |
Staff Manager | Sam Azadi |
Lab Location | Bay 1 |
Tool Manufacturer | Ultratech/Cambridge |
Tool Model | S200 |
NEMO Designation | {{{NEMO_Designation}}} |
Lab Phone | 215-898-9736 |
SOP Link | QNF SOP |
Description
The QNF Savannah ALD is equipped with high-speed pneumatic pulse valves to enable our unique Exposure Mode™ for thin film deposition on ultra high aspect ratio substrates. This proven precision thin film coating methodology can be used to deposit conformal, uniform films on substrates with aspect ratios of greater than > 2000:1.
The QNF Savannah ALD is capable of holding substrates of different sizes (up to 200mm). The system is equipped with six precursor lines for deposition of Al2O3, HfO2, TiO2, and SiO2.
Applications
- Aluminum oxide deposition
- Silicon dioxide deposition
- Titanium oxide deposition
- Hafnium oxide deposition
- Deposition of other films can be made available upon request
Allowed material in ALD System
- Si, SixNy, SiO2, SOI
- Hard masks compatible with process temperature
Resources
SOPs & Troubleshooting
Protocols and Reports
Most Recent Deposition Rate
Material Name | Precursor 1 | Precursor 2 | Dep. temperature [C] | Carrier flow [sccm] | Dep. rate [A/cyc] | Date [MM/DD/YY] | ||||
---|---|---|---|---|---|---|---|---|---|---|
Name | Pulse time [s] | Wait time [s] | Name | Pulse time [s] | Wait time [s] | |||||
Al2O3 | TMA | 0.015 | 5 | H2O | 0.015 | 5 | 200 | 20 | 1 | 09/24/22 |
HfO2 | TDMAHf | 0.15 | 8 | H2O | 0.015 | 5 | 200 | 20 | 1.3 | 09/24/22 |
TiO2 | TDMATi | 0.4 | 10 | H2O | 0.015 | 5 | 250 | 20 | 0.4 | 05/02/22 |