=== Standard process data - Table temperature fixed at 350 C === | === Standard process data - Table temperature fixed at 350 C === | ||
| − | * | + | * SiO<sub>2</sub> on 10/10/2025 |
Recipe parameters: optimized process parameters are in the report under "Protocols and Reports" section | Recipe parameters: optimized process parameters are in the report under "Protocols and Reports" section | ||
| Line 75: | Line 75: | ||
Recipe name on the tool: Test-SiO2 | Recipe name on the tool: Test-SiO2 | ||
| − | Deposition rate: ~ | + | Deposition rate: ~ 323.17 nm/min ± 1.75 nm/min |
| Line 100: | Line 100: | ||
==== Deposition Rate Monitoring ==== | ==== Deposition Rate Monitoring ==== | ||
[[Image:Sio2 dep on cvd-01.jpg|left|500px]] [[Image:Sinx dep rate on cvd-01.jpg|center|500px]] | [[Image:Sio2 dep on cvd-01.jpg|left|500px]] [[Image:Sinx dep rate on cvd-01.jpg|center|500px]] | ||
| − | |||
=== Special process data - adjustable table temperature === | === Special process data - adjustable table temperature === | ||
Revision as of 12:47, 21 October 2025
| Tool Name | Oxford PlasmaLab 100 PECVD |
|---|---|
| Instrument Type | Deposition |
| Staff Manager | Lucas Barreto |
| Lab Location | Bay 1 |
| Tool Manufacturer | Oxford |
| Tool Model | PlasmaLab 100 |
| NEMO Designation | CVD-01 |
| Nearest Phone | 215-898-9736 |
| SOP Link | QNF SOP |
Description
The QNF Oxford Instruments PlasmaLab System 100 Plasma Enhanced Chemical Vapor Deposition (PECVD) tool is used to deposit a variety of thin-film materials at relatively modest temperatures on a variety of substrate materials. The tool utilizes an RF generator to deposit thin films at temperatures lower than traditional chemical vapor deposition systems. The tool operates between 150 and 350 C.
Applications
- Silicon dioxide deposition
- Silicon nitride deposition
- Amorphous silicon deposition
Allowed material in PECVD System
- Si, SixNy, SiO2, SOI, SiC, GaN
- Al, Pt, Cr, W, Mo, Ti
- Hard masks compatible with process temperature
List of materials NOT allowed in the chamber
| Name | symbol | Melting Point [C] |
|---|---|---|
| Bismuth | Bi | 271 |
| Cadmium | Cd | 321 |
| Carbon | C | Subl. |
| Gallium | Ga | 30 |
| Gold | Au | 1062 |
| Indium | In | 157 |
| Lead | Pb | 328 |
| Lithium | Li | 179 |
| Selenium | Se | 217 |
| Sulfur | S | 115 |
| Tellurium | Te | 452 |
| Thallium | Tl | 302 |
| Tin | Sn | 232 |
| Zinc | Zn | 419 |
Process information
Standard process data - Table temperature fixed at 350 C
- SiO2 on 10/10/2025
Recipe parameters: optimized process parameters are in the report under "Protocols and Reports" section
Recipe name on the tool: Test-SiO2
Deposition rate: ~ 323.17 nm/min ± 1.75 nm/min
- SiNx on 07/29/2024
Recipe parameters: optimized process parameters are in the report under "Protocols and Reports" section
Recipe name on the tool: Test-SiNx deposition
Deposition rate: ~ 46 nm/min ± 2 nm/min
- a-Si on 01/09/2024
Recipe parameters: optimized process parameters are in the report under "Protocols and Reports" section
Recipe name on the tool: a-Si
Deposition rate: ~ 60 nm/min ± 5 nm/min
Deposition Rate Monitoring
Special process data - adjustable table temperature
- SiO2
Recipe parameters: optimized process parameters are in the report under "Protocols and Reports" section - table temperature at 200 C
Recipe name on the tool: Test-SiO2
Deposition rate: ~ 230 nm/min ± 2 nm/min