Difference between revisions of "Oxford 80 Plus RIE"
Jump to navigation
Jump to search
| Line 52: | Line 52: | ||
* [https://repository.upenn.edu/scn_tooldata/40/ Reactive Ion Etching (RIE) selectivity of silicon and ZEP520A resist using tetrafluoromethane (CF<sub>4</sub>)] | * [https://repository.upenn.edu/scn_tooldata/40/ Reactive Ion Etching (RIE) selectivity of silicon and ZEP520A resist using tetrafluoromethane (CF<sub>4</sub>)] | ||
| + | |||
| + | |||
| + | ==== Etch Rate ==== | ||
| + | Recipe parameters are defined in the reports above. | ||
| + | |||
| + | * Etch rate of PECVD oxide and nitride are listed in the reports above. | ||
| + | * Etch rate of thermal SiO2 using CF4 recipe: 48 nm/min | ||
| + | * Etch rate of thermal SiO2 using CHF3/O2 recipe: 45 nm/min | ||
| + | * Etch rate of LPCVD SiNx using CF4 recipe: 50 nm/min | ||
| + | * Etch rate of LPCVD SiNx using CHF3/O2 recipe: 57 nm/min | ||
Revision as of 14:51, 3 October 2022
| Tool Name | Oxford 80 Plus RIE |
|---|---|
| Instrument Type | Etch |
| Staff Manager | Sam Azadi |
| Lab Location | Bay 2 |
| Tool Manufacturer | Oxford Instruments |
| Tool Model | 80+ |
| NEMO Designation | {{{NEMO_Designation}}} |
| Nearest Phone | 215-898-9748 |
| SOP Link | QNF SOP |
Description
Oxford 80 Plus is an anisotropic dry etch tool. The main use of this tool is to etch SiO2, and SiNx to create hard masks for deep Si etch. However, it etches many other materials, including a variety of resists. The tool is connected to the following gases: Ar, O2, CF4, CHF3, SF6.
The plasma is ignited by the oscillating electric field created by the RF power at 13.56 MHz. The wafer is cooled down via passive cooling through a graphite chuck.
Applications
- Etch of SiO2
- Etch of SiNx
- Etch of Si
- Etch of resist
Resources
SOPs & Troubleshooting
Protocols and Reports
Etch Rate
Recipe parameters are defined in the reports above.
- Etch rate of PECVD oxide and nitride are listed in the reports above.
- Etch rate of thermal SiO2 using CF4 recipe: 48 nm/min
- Etch rate of thermal SiO2 using CHF3/O2 recipe: 45 nm/min
- Etch rate of LPCVD SiNx using CF4 recipe: 50 nm/min
- Etch rate of LPCVD SiNx using CHF3/O2 recipe: 57 nm/min