Difference between revisions of "Cu master recipe"

From Quattrone Nanofabrication Facility
Jump to navigation Jump to search
(Cu master recipe)
 
 
(2 intermediate revisions by the same user not shown)
Line 1: Line 1:
[[Denton_Explorer14_Magnetron_Sputterer | Return to PVD-05 ]]
+
> [[Denton_Explorer14_Magnetron_Sputterer#Process_data_&_master_recipes | Click here to return to PVD-05]] <
 +
 
 +
Step T004 is the deposition step and step T005 is the cool-down step (300 s).
 +
 
 +
{| class="wikitable"
 +
! Step Number || T000 || T001 || T002 || T003 || T004 || T005 || T006
 +
|-
 +
|-
 +
| Step Time (sec) || 5 || 120  || 60 || 60 || [dep] || 300 || 5
 +
|-style="background-color:#FFFFFF"
 +
| Min Vacuum Setpoint (Torr) ||  ||  ||  ||  ||  ||  ||
 +
|-
 +
|  ||  ||  ||  ||  ||  ||  ||
 +
|-style="background-color:#DBFEFF"
 +
| Gas - (PID or Fixed) ||  ||  PID || PID || PID || PID ||  ||
 +
|-style="background-color:#FFFFFF"
 +
| Gas - PID Master Gas Select ||  || 1 || 1 || 1 || 1 ||  ||
 +
|-
 +
| Gas1 - Setpoint (sccm) ||  ||  10 || 10 || 10 || 10 ||  ||
 +
|-style="background-color:#FFFFFF"
 +
| Gas2 - Setpoint (sccm) ||  ||  ||  ||  ||  ||  ||
 +
|-
 +
|  ||  ||  ||  ||  ||  ||  ||
 +
|-style="background-color:#DEB4DC"
 +
|Gas PID Pressure (mTorr) ||  ||  10 || 5 || 3 || 3 ||  ||
 +
|-style="background-color:#DCF5E9"
 +
| RF Source - Sputter (Watts) ||  ||  ||  ||  ||  ||  ||
 +
|-style="background-color:#DCF5E9"
 +
| RF Source - Cathode Select ||  ||  ||  ||  ||  ||  ||
 +
|-style="background-color:#DCF5E9"
 +
| RF Source - Shutter ||  ||  ||  ||  ||  ||  ||
 +
|-style="background-color:#ECFA6F"
 +
| DC 1 Source - Sputter (Watts) ||  ||  ||  ||  ||  ||  ||
 +
|-style="background-color:#ECFA6F"
 +
| DC 1 Source - Cathode Select ||  ||  ||  ||  ||  ||  ||
 +
|-style="background-color:#ECFA6F"
 +
| DC 1 Source - Shutter ||  ||  ||  ||  ||  ||  ||
 +
|-style="background-color:#FAD86F"
 +
| DC 2 Source - Sputter (Watts) ||  ||  100 || 200 || 300 || 400 ||  ||
 +
|-style="background-color:#FAD86F"
 +
|  ||  ||  ||  ||  ||  ||  ||
 +
|-style="background-color:#FAD86F"
 +
| DC 2 Source - Shutter ||  ||  ||  ||  || Open ||  ||
 +
|-style="background-color:#6FD2FA"
 +
| Pressure Control (Throttle) ||  ||  Yes || Yes || Yes || Yes ||  ||
 +
|-style="background-color:#FFFFFF"
 +
| Ignition Pressure (mTorr) ||  ||  ||  ||  ||  ||  ||
 +
|-
 +
|  ||  ||  ||  ||  ||  ||  ||
 +
|-style="background-color:#E8F213"
 +
| Rotation Speed (0-100%) ||  ||  50 || 50 || 50 || 50 || 50 ||
 +
|-
 +
| End Process (Yes) ||  ||  ||  ||  ||  ||  || Yes
 +
|}

Latest revision as of 15:02, 30 January 2023

> Click here to return to PVD-05 <

Step T004 is the deposition step and step T005 is the cool-down step (300 s).

Step Number T000 T001 T002 T003 T004 T005 T006
Step Time (sec) 5 120 60 60 [dep] 300 5
Min Vacuum Setpoint (Torr)
Gas - (PID or Fixed) PID PID PID PID
Gas - PID Master Gas Select 1 1 1 1
Gas1 - Setpoint (sccm) 10 10 10 10
Gas2 - Setpoint (sccm)
Gas PID Pressure (mTorr) 10 5 3 3
RF Source - Sputter (Watts)
RF Source - Cathode Select
RF Source - Shutter
DC 1 Source - Sputter (Watts)
DC 1 Source - Cathode Select
DC 1 Source - Shutter
DC 2 Source - Sputter (Watts) 100 200 300 400
DC 2 Source - Shutter Open
Pressure Control (Throttle) Yes Yes Yes Yes
Ignition Pressure (mTorr)
Rotation Speed (0-100%) 50 50 50 50 50
End Process (Yes) Yes