Difference between revisions of "Cambridge Nanotech S200 ALD"
Jump to navigation
Jump to search
| (54 intermediate revisions by 5 users not shown) | |||
| Line 1: | Line 1: | ||
| − | [[Category:Deposition]] | + | [[Category:Deposition]][[Category:Atomic Layer Deposition]][[Category:Equipment]] |
{{EquipmentInfo | {{EquipmentInfo | ||
| Line 7: | Line 7: | ||
| imagecaption = | | imagecaption = | ||
| Instrument_Type = Deposition | | Instrument_Type = Deposition | ||
| − | | Staff_Manager = | + | | Staff_Manager = [[Lucas Barreto | Lucas Barreto]] |
| Lab_Location = Bay 1 | | Lab_Location = Bay 1 | ||
| Tool_Manufacturer = Ultratech/Cambridge | | Tool_Manufacturer = Ultratech/Cambridge | ||
| Tool_Model = S200 | | Tool_Model = S200 | ||
| − | | | + | | NEMO_Designation = ALD-01 |
| Lab_Phone = 215-898-9736 | | Lab_Phone = 215-898-9736 | ||
| SOP Link = [https://repository.upenn.edu/scn_sop/6/ QNF SOP] | | SOP Link = [https://repository.upenn.edu/scn_sop/6/ QNF SOP] | ||
| Line 19: | Line 19: | ||
The QNF Savannah ALD is equipped with high-speed pneumatic pulse valves to enable our unique Exposure Mode™ for thin film deposition on ultra high aspect ratio substrates. This proven precision thin film coating methodology can be used to deposit conformal, uniform films on substrates with aspect ratios of greater than > 2000:1. | The QNF Savannah ALD is equipped with high-speed pneumatic pulse valves to enable our unique Exposure Mode™ for thin film deposition on ultra high aspect ratio substrates. This proven precision thin film coating methodology can be used to deposit conformal, uniform films on substrates with aspect ratios of greater than > 2000:1. | ||
| − | The QNF Savannah ALD is capable of holding substrates of different sizes (up to 200mm). The system is equipped with six precursor lines for deposition of Al<sub>2</sub>O<sub>3</sub>, HfO<sub>2</sub>, | + | The QNF Savannah ALD is capable of holding substrates of different sizes (up to 200mm). The system is equipped with six precursor lines for deposition of Al<sub>2</sub>O<sub>3</sub>, HfO<sub>2</sub>, SiO<sub>2</sub>, and TiO<sub>2</sub>. |
===== Applications ===== | ===== Applications ===== | ||
| − | * Aluminum | + | * [[ALD-01: Aluminum Oxide Deposition | Aluminum Oxide Deposition]] |
| − | * | + | * [[ALD-01: Hafnium Oxide Deposition | Hafnium Oxide Deposition]] |
* Titanium oxide deposition | * Titanium oxide deposition | ||
| − | * | + | * [[SiO2 (silicon_dioxide) | Silicon Dioxide deposition]] |
* Deposition of other films can be made available upon request | * Deposition of other films can be made available upon request | ||
| Line 31: | Line 31: | ||
* Si, Si<sub>x</sub>N<sub>y</sub>, SiO<sub>2</sub>, SOI | * Si, Si<sub>x</sub>N<sub>y</sub>, SiO<sub>2</sub>, SOI | ||
* Hard masks compatible with process temperature | * Hard masks compatible with process temperature | ||
| − | |||
== Process Data == | == Process Data == | ||
| Line 41: | Line 40: | ||
{| class="wikitable" | {| class="wikitable" | ||
! rowspan=2 |Material Name | ! rowspan=2 |Material Name | ||
| − | ! colspan= | + | ! colspan=4 |Precursor 1 |
! colspan =3 |Precursor 2 | ! colspan =3 |Precursor 2 | ||
! rowspan=2 |Dep. temperature [C] | ! rowspan=2 |Dep. temperature [C] | ||
| Line 48: | Line 47: | ||
!rowspan=2 |Date [MM/DD/YY] | !rowspan=2 |Date [MM/DD/YY] | ||
|- | |- | ||
| − | ! Name || Pulse time [s] || Wait time [s] || Name || Pulse time [s] || Wait time [s] | + | ! Name || Pulse time [s] || Wait time [s] || Cylinder lot # || Name || Pulse time [s] || Wait time [s] |
| + | |- | ||
| + | | Al<sub>2</sub>O<sub>3</sub> || TMA || 0.015 || 5 || L00222112 || H<sub>2</sub>O || 0.015 || 5 || 150 || 20 || 1.0 || 09/26/25 | ||
| + | |- | ||
| + | | Al<sub>2</sub>O<sub>3</sub> || TMA || 0.015 || 5 || L00222112 || H<sub>2</sub>O || 0.015 || 5 || 245 || 20 || 1.0 || 08/01/25 | ||
|- | |- | ||
| − | | Al<sub>2</sub>O<sub>3</sub> || TMA || 0.015 || 5 || H<sub>2</sub>O || 0.015 || 5 || 200 || 20 || 1 || 09/24/22 | + | | Al<sub>2</sub>O<sub>3</sub> || TMA || 0.015 || 5 || L00222112 || H<sub>2</sub>O || 0.015 || 5 || 245 || 20 || 1.0 || 03/19/25 |
| + | |- | ||
| + | | Al<sub>2</sub>O<sub>3</sub> || TMA || 0.015 || 5 || L00222112 || H<sub>2</sub>O || 0.015 || 5 || 245 || 20 || 1.0 || 11/21/24 | ||
| + | |- | ||
| + | | Al<sub>2</sub>O<sub>3</sub> || TMA || 0.015 || 5 || L00222112 || H<sub>2</sub>O || 0.015 || 5 || 245 || 20 || 1.0 || 8/1/25 | ||
| + | |- | ||
| + | | Al<sub>2</sub>O<sub>3</sub> || TMA || 0.015 || 5 || - || H<sub>2</sub>O || 0.015 || 5 || 200 || 20 || 1 || 09/24/22 | ||
| + | |- | ||
| + | | Al<sub>2</sub>O<sub>3</sub> || TMA || 0.020 || 5 || - || H<sub>2</sub>O || 0.020 || 5 || 150 || 20 || 1 || 02/09/24 | ||
|- | |- | ||
| − | | HfO<sub>2</sub> || TDMAHf || 0. | + | | HfO<sub>2</sub> || TDMAHf || 0.4 || 10 || - || H<sub>2</sub>O || 0.015 || 10 || 200 || 20 || 1.3 || 10/24/25 |
|- | |- | ||
| − | | HfO<sub>2</sub> || TDMAHf || 0. | + | | HfO<sub>2</sub> || TDMAHf || 0.15 || 8 || - || H<sub>2</sub>O || 0.015 || 5 || 200 || 20 || 1.3 || 09/24/22 |
|- | |- | ||
| − | | TiO<sub>2</sub> || TDMATi || 0.4 || 10 || H<sub>2</sub>O || 0.015 || 5 || 250 || 20 || 0.4 || 05/02/22 | + | | HfO<sub>2</sub> || TDMAHf || 0.3 || 10 || - || H<sub>2</sub>O || 0.015 || 8 || 150 || 20 || 1.3 || 04/25/23 |
| + | |- | ||
| + | | TiO<sub>2</sub> || TDMATi || 0.4 || 10 || - || H<sub>2</sub>O || 0.015 || 5 || 250 || 20 || 0.4 || 05/02/22 | ||
| + | |- | ||
| + | | TiO<sub>2</sub> || TDMATi || 0.3 || 10 || - || H<sub>2</sub>O || 0.015 || 10 || 150 || 20 || 0.5 || 02/02/24 | ||
|- | |- | ||
|} | |} | ||
* Ozone based depositions | * Ozone based depositions | ||
| + | Recipe name: 200C_SiO2_qnf_wiki | ||
{| class="wikitable" | {| class="wikitable" | ||
! rowspan=2 |Material Name | ! rowspan=2 |Material Name | ||
| Line 72: | Line 88: | ||
! Name || Pulse time [s] || Wait time [s] : Stop Valve closed / open || Name || Pulse time [s] || Wait time [s] : Stop Valve closed / open | ! Name || Pulse time [s] || Wait time [s] : Stop Valve closed / open || Name || Pulse time [s] || Wait time [s] : Stop Valve closed / open | ||
|- | |- | ||
| − | | SiO<sub>2</sub> || BDEAS || 0. | + | | SiO<sub>2</sub> || BDEAS || 0.05 || 5 SV closed/ 3 SV open || O<sub>3</sub> || 0.2 || 20 SV closed/ 5 SV open || 200 || 20 || 0.6 || 4/23/25 |
|- | |- | ||
|} | |} | ||
| Line 79: | Line 95: | ||
[[Image:Hafnia Oct6.jpg|left|500px]] [[Image:Alumina Oct6.jpg|center|500px]] | [[Image:Hafnia Oct6.jpg|left|500px]] [[Image:Alumina Oct6.jpg|center|500px]] | ||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
| − | |||
== Resources == | == Resources == | ||
| Line 118: | Line 100: | ||
===== SOPs & Troubleshooting ===== | ===== SOPs & Troubleshooting ===== | ||
* [https://repository.upenn.edu/scn_sop/6/ QNF SOP] | * [https://repository.upenn.edu/scn_sop/6/ QNF SOP] | ||
| + | * [https://upenn.box.com/s/3hq8iik8jeb1385mrwgs16i6vfpvxt6f ALD KOH Cleaning Procedure] | ||
| + | |||
===== Protocols and Reports ===== | ===== Protocols and Reports ===== | ||
* [https://repository.upenn.edu/scn_protocols/72/ ALD deposition of SiO<sub>2</sub> using BDEAS and Ozone precursors] | * [https://repository.upenn.edu/scn_protocols/72/ ALD deposition of SiO<sub>2</sub> using BDEAS and Ozone precursors] | ||
Latest revision as of 15:23, 24 October 2025
| Tool Name | Cambridge Nanotech S200 ALD |
|---|---|
| Instrument Type | Deposition |
| Staff Manager | Lucas Barreto |
| Lab Location | Bay 1 |
| Tool Manufacturer | Ultratech/Cambridge |
| Tool Model | S200 |
| NEMO Designation | ALD-01 |
| Nearest Phone | 215-898-9736 |
| SOP Link | QNF SOP |
Description
The QNF Savannah ALD is equipped with high-speed pneumatic pulse valves to enable our unique Exposure Mode™ for thin film deposition on ultra high aspect ratio substrates. This proven precision thin film coating methodology can be used to deposit conformal, uniform films on substrates with aspect ratios of greater than > 2000:1.
The QNF Savannah ALD is capable of holding substrates of different sizes (up to 200mm). The system is equipped with six precursor lines for deposition of Al2O3, HfO2, SiO2, and TiO2.
Applications
- Aluminum Oxide Deposition
- Hafnium Oxide Deposition
- Titanium oxide deposition
- Silicon Dioxide deposition
- Deposition of other films can be made available upon request
Allowed material in ALD System
- Si, SixNy, SiO2, SOI
- Hard masks compatible with process temperature
Process Data
Standard Processes
- Water based depositions
| Material Name | Precursor 1 | Precursor 2 | Dep. temperature [C] | Carrier flow [sccm] | Dep. rate [A/cyc] | Date [MM/DD/YY] | |||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Name | Pulse time [s] | Wait time [s] | Cylinder lot # | Name | Pulse time [s] | Wait time [s] | |||||
| Al2O3 | TMA | 0.015 | 5 | L00222112 | H2O | 0.015 | 5 | 150 | 20 | 1.0 | 09/26/25 |
| Al2O3 | TMA | 0.015 | 5 | L00222112 | H2O | 0.015 | 5 | 245 | 20 | 1.0 | 08/01/25 |
| Al2O3 | TMA | 0.015 | 5 | L00222112 | H2O | 0.015 | 5 | 245 | 20 | 1.0 | 03/19/25 |
| Al2O3 | TMA | 0.015 | 5 | L00222112 | H2O | 0.015 | 5 | 245 | 20 | 1.0 | 11/21/24 |
| Al2O3 | TMA | 0.015 | 5 | L00222112 | H2O | 0.015 | 5 | 245 | 20 | 1.0 | 8/1/25 |
| Al2O3 | TMA | 0.015 | 5 | - | H2O | 0.015 | 5 | 200 | 20 | 1 | 09/24/22 |
| Al2O3 | TMA | 0.020 | 5 | - | H2O | 0.020 | 5 | 150 | 20 | 1 | 02/09/24 |
| HfO2 | TDMAHf | 0.4 | 10 | - | H2O | 0.015 | 10 | 200 | 20 | 1.3 | 10/24/25 |
| HfO2 | TDMAHf | 0.15 | 8 | - | H2O | 0.015 | 5 | 200 | 20 | 1.3 | 09/24/22 |
| HfO2 | TDMAHf | 0.3 | 10 | - | H2O | 0.015 | 8 | 150 | 20 | 1.3 | 04/25/23 |
| TiO2 | TDMATi | 0.4 | 10 | - | H2O | 0.015 | 5 | 250 | 20 | 0.4 | 05/02/22 |
| TiO2 | TDMATi | 0.3 | 10 | - | H2O | 0.015 | 10 | 150 | 20 | 0.5 | 02/02/24 |
- Ozone based depositions
Recipe name: 200C_SiO2_qnf_wiki
| Material Name | Precursor 1 | Precursor 2 | Dep. temperature [C] | Carrier flow [sccm] | Dep. rate [A/cyc] | Date [MM/DD/YY] | ||||
|---|---|---|---|---|---|---|---|---|---|---|
| Name | Pulse time [s] | Wait time [s] : Stop Valve closed / open | Name | Pulse time [s] | Wait time [s] : Stop Valve closed / open | |||||
| SiO2 | BDEAS | 0.05 | 5 SV closed/ 3 SV open | O3 | 0.2 | 20 SV closed/ 5 SV open | 200 | 20 | 0.6 | 4/23/25 |