Difference between revisions of "Heidelberg DWL 66+ Laser Writer"

From Quattrone Nanofabrication Facility
Jump to navigation Jump to search
 
(65 intermediate revisions by 2 users not shown)
Line 1: Line 1:
[[Category:Lithography]]
+
[[Category:Lithography]][[Category:Photolithography]][[Category:Equipment]]
  
 
{{EquipmentInfo
 
{{EquipmentInfo
 
| name = Heidelberg DWL 66+ Laser Writer
 
| name = Heidelberg DWL 66+ Laser Writer
 
| Tool_Name = Heidelberg DWL 66+ Laser Writer
 
| Tool_Name = Heidelberg DWL 66+ Laser Writer
| image = [[Image:LW-01.jpeg|300px]]
+
| image = [[Image:LW-01.jpeg|250px]]
 
| imagecaption =  
 
| imagecaption =  
 
| Instrument_Type = Lithography
 
| Instrument_Type = Lithography
| Staff_Manager = David Jones
+
| Staff_Manager = [[Ana Cohen | Ana Cohen]]
| Lab_Location = Bay 2
+
| Lab_Location = Bay 4
 
| Tool_Manufacturer = Heidelberg  
 
| Tool_Manufacturer = Heidelberg  
 
| Tool_Model = DWL 66+
 
| Tool_Model = DWL 66+
| Iris_Designation = LW-01
+
| NEMO_Designation = LW-01
 
| Lab_Phone = 8-9799
 
| Lab_Phone = 8-9799
| SOP Link = [https://repository.upenn.edu/scn_protocols/76/ SOP]
+
| SOP Link = [https://nemo.nano.upenn.edu/media/tool_documents/lw-01-heidelberg-dwl66/LW-01_SOP_v02.pdf SOP]
 
}}
 
}}
  
 
== Description ==
 
== Description ==
The fully automated DWL 66+ laser writing system is located inside an environment chamber for stable environment of the system with controlled laminar airflow and temperature stability. The chamber is situated on a granite base with air cushions for vibration isolation. The optical system includes highly reflective mirrors and acousto-optic modulators for real-time beam correction.  
+
The fully automated DWL 66+ laser writing system has both binary (2D) and grayscale (2.5D) exposure capability.
 +
[[File: DWL schematic.PNG|thumb|right|upright=0.75|Schematic of pattern exposure with the DWL66+, [https://heidelberg-instruments.com/wp-content/uploads/2025/05/The-Lithographer-Surface-Issue.pdf TheLithographer.com, Surface Issue, May 2025] ]]
 +
The pattern is broken into vertical stripes of ~500px with preset overlap. To write each stripe, the tool modulates and deflects the laser beam based on the provided pattern data while the stage moves along Y. This process repeats along the X direction until the pattern is complete.
  
'''Lens & Resolution'''
+
== Allowed Materials ==
* 2 mm lens (optical autofocus): 600 nm
+
Substrates
* 10 mm lens (pneumatic autofocus): 2 µm
+
* Mask Plates -- available in the [https://nemo.nano.upenn.edu/stockroom/ QNF Stockroom] pre-coated with AZ1500 and IP3500
* 40 mm lens (pneumatic autofocus): 10 µm
+
* 4" wafers
 
+
* Pieceparts > 20mm x 20mm ''(Starting Aug 2025, DMO system is recommended for small piece part direct write)  
 
+
Resists -- must be compatible with h-line/ 405nm exposure ''(Laser exchanged in June 2023. Previous documentation may include 365nm capability.)''
===== Applications =====
+
* [[Resists_at_QNF#QNF_Supplied_Standard_Photoresists | S1800 series]]
* Patterning of photomasks
+
* [[Resists_at_QNF#Miscellaneous | KL5300 series]]
* Direct laser writing of patterns
+
* [[Resists_at_QNF#Other_Resists | LOR]]
  
 
== Processes ==
 
== Processes ==
The following exposure parameters may be used to expose photomasks.
+
=== Writehead Selection ===
 +
<u><small>'''NOTE</u>:'''</small>'' Pneumatic mode not currently recommended for dry etch and features under 10x listed minimum feature size due to focus issues -- working with Heidelberg service to address. </br> Last confirmed November 2025.''
 
{| class="wikitable" style="vertical-align:bottom;"
 
{| class="wikitable" style="vertical-align:bottom;"
 
|-
 
|-
! Resist
 
 
! Write Head
 
! Write Head
! Filter(s)
+
! Optical Focus
! Laser Power (mW)
+
! Pneumatic Focus
! Intensity
+
! Minimum Feature Size
! Focus
 
! Focus mode
 
 
|-
 
|-
| AZ1500
 
 
| 10mm
 
| 10mm
| 50%
+
| -60
| 50
+
| -100
| 70%
+
| 2um
| -10
 
| Pnematic
 
 
|-
 
|-
| IP3500
+
| 2mm
| 10mm
+
| +50
| None
+
| -100
| 50
+
| 600nm
| 90%
 
| -10
 
| Pnematic
 
 
|-
 
|-
| IP3500
+
| 40mm
| 2mm
+
| N/A
| 12.5%
+
| -100
| 50
+
| 10um
| 30%
 
| -30
 
| Pnematic
 
 
|}
 
|}
  
 
+
===Exposure Parameters===
The following exposure parameters may be used to direct write into S1800 resist (soft baked at 115C for 1 minute) with the 10mm write head. For the optimum focus, please refer to the "AZ1500.txt" or "IP3500.txt" files for the optimum value to use.
+
=====Mask Plates=====
 
+
[[File: 10mm n70opt 4.jpg|thumb|right|upright=0.75| 2um lines on AZ1500 using 10mm with optical focus (June 2025)]]
 +
''530nm resist thickness on chrome-coated soda lime, purchased from TELIC. Development in TMAH 0.26N for 60s. Values last confirmed July 2025.''
 +
======AZ1500======
 +
''Lower contrast resist - the default option for most applications''
 
{| class="wikitable" style="vertical-align:bottom;"
 
{| class="wikitable" style="vertical-align:bottom;"
 
|-
 
|-
! Resist thk  (µm)
+
! Write Head
! Laser power (mW)
+
! Filter(s)
 +
! Laser Power
 
! Intensity
 
! Intensity
! Filter
 
 
|-
 
|-
| 0.50
+
| 10mm
| 28.83
 
| 100%
 
 
| 50%
 
| 50%
 +
| 60 mW
 +
| 90
 
|-
 
|-
| 0.55
+
| 2mm
| 29.53
+
| 12.5% + 25%
| 100%
+
| 60 mW
| 50%
+
| 80
 
|-
 
|-
| 0.60
+
| 40mm
| 30.33
+
| NONE
| 100%
+
| 220 mW
| 50%
+
| 60
 +
|}
 +
======IP3500======
 +
''Higher contrast resist - produces better corners and small pitch gratings''
 +
{| class="wikitable" style="vertical-align:bottom;"
 
|-
 
|-
| 0.65
+
! Write Head
| 31.25
+
! Filter(s)
| 100%
+
! Laser Power
| 50%
+
! Intensity
 
|-
 
|-
| 0.70
+
| 10mm
| 32.28
+
| NONE
| 100%
+
| 120 mW
| 50%
+
| 90
 
|-
 
|-
| 0.75
+
| 2mm
| 33.41
+
| 12.5% + 50%
| 100%
+
| 60 mW
| 50%
+
| 80
 +
|}
 +
 
 +
=====Other direct writes=====
 +
[[File: LW-01 S1818Lines 25um Feb2024.png|thumb|right|upright=0.75| 5um, 10um, 25um, and 50um lines using 10mm writehead on 2um S1818 (Feb 2024)]]
 +
''Resist on 4" silicon wafer, soft baked at 115C for 60s, development in TMAH 0.26N for 60s. '' <br>
 +
<u><small>'''NOTE</u>:'''</small> Even if your resist is listed here, a dose test is always recommended to confirm optimal exposure parameters due to the variability of resist thickness, substrate reflectivity, and the ideal profile for subsequent processes.
 +
{| class="wikitable"
 
|-
 
|-
| 0.80
+
! Resist
| 34.66
+
! Thickness/<br>Spin Speed
| 100%
+
! Write Head
| 50%
+
! Filter(s)
 +
! Laser Power
 +
! Intensity
 
|-
 
|-
| 0.85
+
| S1805
| 36.03
+
| 0.5um (3krpm)
| 100%
+
| 10mm
 
| 50%
 
| 50%
 +
| 60 mW
 +
| 70
 
|-
 
|-
| 0.90
+
| S1818
| 37.50
+
| 2.2um (3krpm)
| 100%
+
| 10mm
| 50%
+
| NONE
|-
+
| 130 mW
| 0.95
+
| 100
| 39.08
 
| 100%
 
| 50%
 
|-
 
| 1.00
 
| 40.78
 
| 100%
 
| 50%
 
|-
 
| 1.05
 
| 42.58
 
| 100%
 
| 50%
 
|-
 
| 1.10
 
| 44.50
 
| 100%
 
| 50%
 
|-
 
| 1.15
 
| 46.53
 
| 100%
 
| 50%
 
|-
 
| 1.20
 
| 48.67
 
| 100%
 
| 50%
 
|-
 
| 1.25
 
| 50.92
 
| 100%
 
| 50%
 
|-
 
| 1.30
 
| 53.28
 
| 100%
 
| 50%
 
|-
 
| 1.35
 
| 55.75
 
| 100%
 
| 50%
 
|-
 
| 1.40
 
| 58.34
 
| 100%
 
| 50%
 
|-
 
| 1.45
 
| 61.03
 
| 100%
 
| 50%
 
|-
 
| 1.50
 
| 63.84
 
| 100%
 
| 50%
 
 
|}
 
|}
  
 +
== Resources ==
 +
===== SOPs =====
 +
* [https://nemo.nano.upenn.edu/media/tool_documents/lw-01-heidelberg-dwl66/LW-01_SOP_v02.pdf SOP]
 +
* [https://www.youtube.com/watch?v=q_mvEGSCEGI&list=PLiihbHV9HgpWAcmgdpMGBkejcBhEzoKJO Videos - LW-01 Tool Training]
 +
* [https://drive.google.com/file/d/1MUMPdLl4GfXtmg3gJjdiPKbdiyCq-elM/view?usp=drive_link Video - Chuck Installation/Removal]
  
The following exposure parameters may be used to direct write into S1800 resist (soft baked at 115C for 1 minute) with the 2mm write head.  For the optimum focus, please refer to the "AZ1500.txt" or "IP3500.txt" files for the optimum value to use.
+
=====Mask Making=====
{| class="wikitable"
+
* [https://nemo.nano.upenn.edu/media/tool_documents/lw-01-heidelberg-dwl66/How_to_Make_a_Mask_At_QNF_v05.pdf How to Make a Mask at QNF]
|- style="vertical-align:bottom;"
+
* [https://rise.articulate.com/share/A8k76vtz0l6qxlA2gDZcYHPmJl5bB2C0#/ Introduction to KLayout (LNF)]
! Resist Thk (µm)
+
* [https://www.youtube.com/playlist?list=PLiihbHV9HgpWZikttBFUh2O8EGUsRu348 BEAMER Training for LW-01]
! Laser Power (mW)
 
! Intensity
 
! Filter
 
|-
 
| style="vertical-align:bottom;" | 0.5
 
| 24.123
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 0.55
 
| 26.421
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 0.6
 
| 28.708
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 0.65
 
| 30.984
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 0.7
 
| 33.249
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 0.75
 
| 35.503
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 0.8
 
| 37.747
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 0.85
 
| 39.979
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 0.9
 
| 42.200
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 0.95
 
| 44.411
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 1
 
| 46.610
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 1.05
 
| 48.799
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 1.1
 
| 50.977
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 1.15
 
| 53.143
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 1.2
 
| 55.299
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 1.25
 
| 57.444
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 1.3
 
| 59.578
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 1.35
 
| 61.701
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 1.4
 
| 63.813
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 1.45
 
| 65.914
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|-
 
| style="vertical-align:bottom;" | 1.5
 
| 68.005
 
| style="vertical-align:bottom;" | 70%
 
| style="vertical-align:bottom;" | 12.5% & 25%
 
|}
 
  
== Resources ==
+
=====Troubleshooting =====
 +
* [https://upenn.box.com/s/9kc3fz6gktrrrlac4e0drmzwjzwmufxl Power Up Instructions]
  
===== SOPs & Troubleshooting =====
+
=====References=====
* [https://repository.upenn.edu/scn_protocols/76/ QNF SOP]
+
* [https://heidelberg-instruments.com/product/dwl-66/ Heidelberg Instruments]

Latest revision as of 17:06, 20 November 2025


Heidelberg DWL 66+ Laser Writer
LW-01.jpeg
Tool Name Heidelberg DWL 66+ Laser Writer
Instrument Type Lithography
Staff Manager Ana Cohen
Lab Location Bay 4
Tool Manufacturer Heidelberg
Tool Model DWL 66+
NEMO Designation LW-01
Nearest Phone 8-9799
SOP Link SOP

Description

The fully automated DWL 66+ laser writing system has both binary (2D) and grayscale (2.5D) exposure capability.

Schematic of pattern exposure with the DWL66+, TheLithographer.com, Surface Issue, May 2025

The pattern is broken into vertical stripes of ~500px with preset overlap. To write each stripe, the tool modulates and deflects the laser beam based on the provided pattern data while the stage moves along Y. This process repeats along the X direction until the pattern is complete.

Allowed Materials

Substrates

  • Mask Plates -- available in the QNF Stockroom pre-coated with AZ1500 and IP3500
  • 4" wafers
  • Pieceparts > 20mm x 20mm (Starting Aug 2025, DMO system is recommended for small piece part direct write)

Resists -- must be compatible with h-line/ 405nm exposure (Laser exchanged in June 2023. Previous documentation may include 365nm capability.)

Processes

Writehead Selection

NOTE: Pneumatic mode not currently recommended for dry etch and features under 10x listed minimum feature size due to focus issues -- working with Heidelberg service to address.
Last confirmed November 2025.

Write Head Optical Focus Pneumatic Focus Minimum Feature Size
10mm -60 -100 2um
2mm +50 -100 600nm
40mm N/A -100 10um

Exposure Parameters

Mask Plates
2um lines on AZ1500 using 10mm with optical focus (June 2025)

530nm resist thickness on chrome-coated soda lime, purchased from TELIC. Development in TMAH 0.26N for 60s. Values last confirmed July 2025.

AZ1500

Lower contrast resist - the default option for most applications

Write Head Filter(s) Laser Power Intensity
10mm 50% 60 mW 90
2mm 12.5% + 25% 60 mW 80
40mm NONE 220 mW 60
IP3500

Higher contrast resist - produces better corners and small pitch gratings

Write Head Filter(s) Laser Power Intensity
10mm NONE 120 mW 90
2mm 12.5% + 50% 60 mW 80
Other direct writes
5um, 10um, 25um, and 50um lines using 10mm writehead on 2um S1818 (Feb 2024)

Resist on 4" silicon wafer, soft baked at 115C for 60s, development in TMAH 0.26N for 60s.
NOTE: Even if your resist is listed here, a dose test is always recommended to confirm optimal exposure parameters due to the variability of resist thickness, substrate reflectivity, and the ideal profile for subsequent processes.

Resist Thickness/
Spin Speed
Write Head Filter(s) Laser Power Intensity
S1805 0.5um (3krpm) 10mm 50% 60 mW 70
S1818 2.2um (3krpm) 10mm NONE 130 mW 100

Resources

SOPs
Mask Making
Troubleshooting
References