Difference between revisions of "Heidelberg DWL 66+ Laser Writer"

From Quattrone Nanofabrication Facility
Jump to navigation Jump to search
Line 37: Line 37:
 
== Processes ==
 
== Processes ==
 
The following exposure parameters may be used to expose photomasks. <em>  </em>
 
The following exposure parameters may be used to expose photomasks. <em>  </em>
 +
 +
{| class="wikitable" style="vertical-align:bottom;"
 +
|-
 +
! Write Head
 +
! Focus
 +
! Mode
 +
! Notes
 +
|-
 +
| 10mm
 +
| -100
 +
| Pneumatic
 +
| active problem, not currently recommended for <25um
 +
|-
 +
| 10mm
 +
| -70
 +
| Optical
 +
| for >2um minimum
 +
|-
 +
| 2mm
 +
| -100
 +
| Pneumatic
 +
| active problem, not currently recommended
 +
|-
 +
| 2mm
 +
| +40
 +
| Optical
 +
| for >600nm minimum
 +
|-
 +
| 40mm
 +
| -100
 +
| Pneumatic
 +
| active problem, not currently recommended
 +
|}
 +
 +
 
{| class="wikitable" style="vertical-align:bottom;"
 
{| class="wikitable" style="vertical-align:bottom;"
 
|-
 
|-
Line 44: Line 79:
 
! Laser Power
 
! Laser Power
 
! Intensity
 
! Intensity
! Focus
+
! Notes
! # of passes
 
! Focus mode
 
 
|-
 
|-
 
| AZ1500
 
| AZ1500
Line 53: Line 86:
 
| 60 mW
 
| 60 mW
 
| 90
 
| 90
| -25
+
|
| 1
 
| Pneumatic
 
 
|-
 
|-
 
| IP3500
 
| IP3500
Line 62: Line 93:
 
| 120 mW
 
| 120 mW
 
| 90
 
| 90
| -25
+
| for <3um
| 1
 
| Pneumatic
 
 
|-
 
|-
 
| AZ1500
 
| AZ1500
Line 71: Line 100:
 
| 60 mW
 
| 60 mW
 
| 80
 
| 80
| +8
 
| 1
 
| Pneumatic
 
 
|-
 
|-
 
| IP3500
 
| IP3500
Line 80: Line 106:
 
| 60 mW
 
| 60 mW
 
| 80
 
| 80
| +8
+
| for <1um
| 1
 
| Pneumatic
 
 
|-
 
|-
 
| AZ1500
 
| AZ1500
Line 89: Line 113:
 
| 220 mW
 
| 220 mW
 
| 60
 
| 60
| 0
 
| 1
 
| Pneumatic
 
|-
 
| IP3500
 
| 40mm
 
| NONE
 
| 220 mW
 
| 60
 
| 0
 
| 4
 
| Pneumatic
 
 
|}
 
|}
  
Line 114: Line 126:
 
! Laser Power
 
! Laser Power
 
! Intensity
 
! Intensity
! # passes
 
! Focus mode
 
 
|-
 
|-
 
| S1805
 
| S1805
Line 123: Line 133:
 
| 60 mW
 
| 60 mW
 
| 70
 
| 70
| 1
 
| pneumatic
 
 
|-
 
|-
 
| S1818
 
| S1818
Line 132: Line 140:
 
| 130 mW
 
| 130 mW
 
| 100
 
| 100
| 1
 
| pneumatic
 
 
|}
 
|}
  

Revision as of 14:36, 17 July 2025


Heidelberg DWL 66+ Laser Writer
LW-01.jpeg
Tool Name Heidelberg DWL 66+ Laser Writer
Instrument Type Lithography
Staff Manager Ana Cohen
Lab Location Bay 4
Tool Manufacturer Heidelberg
Tool Model DWL 66+
NEMO Designation LW-01
Nearest Phone 8-9799
SOP Link SOP

Description

The fully automated DWL 66+ laser writing system is located inside an environment chamber for stable environment of the system with controlled laminar airflow and temperature stability. The chamber is situated on a granite base with air cushions for vibration isolation. The optical system includes highly reflective mirrors and acousto-optic modulators for real-time beam correction. The laser is 405nm wavelength (h-line).

Lens & Resolution

  • 2 mm lens (optical autofocus): 600 nm
  • 10 mm lens (pneumatic autofocus): 2 µm
  • 40 mm lens (pneumatic autofocus): 10 µm
Applications
Allowed Materials

Processes

The following exposure parameters may be used to expose photomasks.

Write Head Focus Mode Notes
10mm -100 Pneumatic active problem, not currently recommended for <25um
10mm -70 Optical for >2um minimum
2mm -100 Pneumatic active problem, not currently recommended
2mm +40 Optical for >600nm minimum
40mm -100 Pneumatic active problem, not currently recommended


Resist Write Head Filter(s) Laser Power Intensity Notes
AZ1500 10mm 50% 60 mW 90
IP3500 10mm NONE 120 mW 90 for <3um
AZ1500 2mm 12.5% + 25% 60 mW 80
IP3500 2mm 12.5% + 50% 60 mW 80 for <1um
AZ1500 40mm NONE 220 mW 60


The following exposure parameters may be used to direct write into S18xx resist on silicon (soft baked at 115C for 60s, development in TMAH 0.26N for 60s). For the optimum focus, please refer to the "AZ1500.txt" or "IP3500.txt" files for the optimum value to use. [May not be up-to-date. It is always a good idea to check your resist thickness and run a dose test to confirm optimal parameters.]

Resist Thickness/Spin Speed Write Head Filter(s) Laser Power Intensity
S1805 0.5um (3krpm) 10mm 50% 60 mW 70
S1818 2.2um (3krpm) 10mm NONE 130 mW 100


 LW-01 S1818Lines 25um Feb2024.png LW-01 S1818Lines 5um Feb2024.png
 S1818 at 3000rpm (2.2um thickness) with 10mm writehead [Feb 2024]
 65mW, NO Filter, 70% intensity, + 20 focus
 5um, 10um, 25um, and 50um line widths after 60s TMAH 0.26N development

Resources