| Line 32: | Line 32: | ||
The following exposure parameters may be used to direct write into S1800 resist (soft baked at 115C for 1 minute) with the 10mm write head. For the optimum focus, please refer to the "AZ1500.txt" or "IP3500.txt" files for the optimum value to use. | The following exposure parameters may be used to direct write into S1800 resist (soft baked at 115C for 1 minute) with the 10mm write head. For the optimum focus, please refer to the "AZ1500.txt" or "IP3500.txt" files for the optimum value to use. | ||
| − | + | {| class="wikitable" style="vertical-align:bottom;" | |
| + | |- | ||
| + | ! Resist thk (µm) | ||
| + | ! Laser power (mW) | ||
| + | ! Intensity | ||
| + | ! Filter | ||
| + | |- | ||
| + | | 0.50 | ||
| + | | 28.83 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 0.55 | ||
| + | | 29.53 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 0.60 | ||
| + | | 30.33 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 0.65 | ||
| + | | 31.25 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 0.70 | ||
| + | | 32.28 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 0.75 | ||
| + | | 33.41 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 0.80 | ||
| + | | 34.66 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 0.85 | ||
| + | | 36.03 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 0.90 | ||
| + | | 37.50 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 0.95 | ||
| + | | 39.08 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 1.00 | ||
| + | | 40.78 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 1.05 | ||
| + | | 42.58 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 1.10 | ||
| + | | 44.50 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 1.15 | ||
| + | | 46.53 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 1.20 | ||
| + | | 48.67 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 1.25 | ||
| + | | 50.92 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 1.30 | ||
| + | | 53.28 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 1.35 | ||
| + | | 55.75 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 1.40 | ||
| + | | 58.34 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 1.45 | ||
| + | | 61.03 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |- | ||
| + | | 1.50 | ||
| + | | 63.84 | ||
| + | | 100% | ||
| + | | 50% | ||
| + | |} | ||
== Resources == | == Resources == | ||
Revision as of 16:00, 23 December 2022
| Tool Name | Heidelberg DWL 66+ Laser Writer |
|---|---|
| Instrument Type | Lithography |
| Staff Manager | David Jones |
| Lab Location | Bay 2 |
| Tool Manufacturer | Heidelberg |
| Tool Model | DWL 66+ |
| NEMO Designation | {{{NEMO_Designation}}} |
| Nearest Phone | 8-9799 |
| SOP Link | SOP |
Description
The fully automated DWL 66+ laser writing system is located inside an environment chamber for stable environment of the system with controlled laminar airflow and temperature stability. The chamber is situated on a granite base with air cushions for vibration isolation. The optical system includes highly reflective mirrors and acousto-optic modulators for real-time beam correction.
Lens & Resolution
- 2 mm lens (optical autofocus): 600 nm
- 10 mm lens (pneumatic autofocus): 2 µm
- 40 mm lens (pneumatic autofocus): 10 µm
Applications
- Patterning of photomasks
- Direct laser writing of patterns
Processes
The following exposure parameters may be used to direct write into S1800 resist (soft baked at 115C for 1 minute) with the 10mm write head. For the optimum focus, please refer to the "AZ1500.txt" or "IP3500.txt" files for the optimum value to use.
| Resist thk (µm) | Laser power (mW) | Intensity | Filter |
|---|---|---|---|
| 0.50 | 28.83 | 100% | 50% |
| 0.55 | 29.53 | 100% | 50% |
| 0.60 | 30.33 | 100% | 50% |
| 0.65 | 31.25 | 100% | 50% |
| 0.70 | 32.28 | 100% | 50% |
| 0.75 | 33.41 | 100% | 50% |
| 0.80 | 34.66 | 100% | 50% |
| 0.85 | 36.03 | 100% | 50% |
| 0.90 | 37.50 | 100% | 50% |
| 0.95 | 39.08 | 100% | 50% |
| 1.00 | 40.78 | 100% | 50% |
| 1.05 | 42.58 | 100% | 50% |
| 1.10 | 44.50 | 100% | 50% |
| 1.15 | 46.53 | 100% | 50% |
| 1.20 | 48.67 | 100% | 50% |
| 1.25 | 50.92 | 100% | 50% |
| 1.30 | 53.28 | 100% | 50% |
| 1.35 | 55.75 | 100% | 50% |
| 1.40 | 58.34 | 100% | 50% |
| 1.45 | 61.03 | 100% | 50% |
| 1.50 | 63.84 | 100% | 50% |